PHYSICAL PROPERTIES

PRODUCT ; PRETREATED POLYESTER FILM
TYPE (CODE) ; FCCO (ANTI-STATIC)
MAIN USAGE ; PACKAGING, MONTAGE FILM

PROPERTIES UNIT TYPICAL VALUES TEST METHOD
Average Thickness §­ 12 100       -
Tensile Strength MD §¸/§±
psi¡¿10©ø
28
39
19
27
      ASTM D-882
TD §¸/§±
psi¡¿10©ø
26
37
21
29
     
Elongation
at break
MD % 130 200       ASTM D-882
TD % 135 135      
F-5 Value MD §¸/§±
psi¡¿10©ø
12
17
12
16
      ASTM D-882
TD §¸/§±
psi¡¿10©ø
11
16
12
16
     
Heat Shrinkage
(in hot air)
MD % 1.2 0.5       ASTM D-2305
(150¡É, 30 min)
TD % 0.0 0.5      
Friction Coefficient
(film/film ; in/out)
¥ìs - 0.31 0.18       ASTM D-1894
¥ìk - 0.37 0.18      
Wetting Tension
(coated ; in)
In dynes/cm 50 50       ASTM D-2578
Out dynes/cm 40 40      
Haze % 2.7 1.3       ASTM D-1003
Surface Resistivity ¥Ø/sq. 1.0¡¿1010                                  ASTM D-257(23¡É, 45%RH)