| PHYSICAL PROPERTIES |
| PRODUCT | ; ADHESION PROMOTED POLYESTER FILM |
| TYPE (CODE) | ; FCGO (FOR WATER BASED OR WATER/ALCOHOL BASED) |
| MAIN USAGE | ; PRINTING, COATING |
| PROPERTIES | UNIT | TYPICAL VALLUES | TEST METHOD | |||||
| Average Thickness | § | 50 | 100 | |||||
| Tensile Strength | MD | §¸/§± psi¡¿10©ø |
20 28 |
19 27 |
ASTMD-882 | |||
| TD | §¸/§± psi¡¿10©ø |
23 33 |
21 30 |
|||||
| Elongation at break |
MD | % | 180 | 200 | ASTMD-882 | |||
| TD | % | 130 | 135 | |||||
| F-5 Value | MD | §¸/§± psi¡¿10©ø |
12 17 |
12 17 |
ASTMD-882 | |||
| TD | §¸/§± psi¡¿10©ø |
11 16 |
12 17 |
|||||
| Heat
Shrinkage (in hot air) |
MD | % | 0.5 | 0.5 | ASTMD-2305 (150¡É, 30 min) |
|||
| TD | % | 0.5 | 0.5 | |||||
| Friction
Coefficient (film/film ; in/out) |
¥ìs | - | 0.24 | 0.29 | ASTMD-1894 | |||
| ¥ìk | - | 0.23 | 0.34 | |||||
| Wetting
Tension (coated ; in) |
In | dynes/cm | 40 | 38 | ASTMD-2578 | |||
| Out | dynes/cm | 40 | 40 | |||||
| Haze | % | 0.8 | 1.3 | ASTMD-1003 | ||||
| Test Condition | ¡¤Normal laboratory ambient condition ; 23¡É, 50% RH | |||||||